ASTM » ASTM F2077

A Guide to ASTM F2077-18, Characterization and Fatigue of Spinal Intervertebral Body Fusion Devices

A SUMMARY OF THE STANDARD AND THE DYNAMIC TESTS REQUIRED

Written by Toby Lane

Intervertebral Body Fusion devices are used to promote arthrodesis of a spinal motion segment, following disc degeneration. The implant acts as a support of the anterior column whilst the two vertebral discs grow together and fuse the spine. Intervertebral Body Fusion is an alternative technique to that of Intervertebral Disc replacement.

The tests include:

  • Axial-Compression
  • Compression-Shear
  • Torsion Testing

We recommend that you review the standard to fully understand its requirements. An alternative test for intervertebral body fusion devices is specified in ASTM-F2267.

 

Test Fixture for Spinal Interbody Fusion Devices to ASTM standards

Challenges of ASTM F2077 Testing:

  • Machining/manufacture of test blocks to match specimen shape
  • Monitoring of intradiscal height during test
  • Assessment of mechanical failure during test
  • Avoidance of self-heating in test blocks
  • Maintaining load peaks at high frequency
  • Test duration for in vivo tests

 

TEST PARAMETERSAll tests must first be run at ambient temperature in air before being repeated in a simulated in vivo condition using a fluid bath and saline solution at 37°C if required. In vivo testing should not be carried out at a frequency higher than 1Hz.

Static Tests Dynamic Tests
Axial-Compression
  • Position controlled test at a rate of ≤25mm/min
  • Test until functional or mechanical failure (sample yielding)
  • Test results for 5 samples must be obtained
  • Load controlled test
  • Test run to functional or mechanical failure or 5 million cycles
  • Frequency can be determined by the user but must avoid self-heating of the polyacetal tests blocks and specimen. Typically values range from 5–30 Hz in air and up to 1 Hz for in vivo conditions
  • An R ratio of 10 is used (e.g. between 100 N and 1000 N)
  • The maximum test force should represent either 25%, 50% or 75% of the sample yield strength determined from the static tests. Typical maximum forces can be in excess of 2500N
  • Samples should be examined without removal at regular intervals during the tests to check for mechanical failures
Compression-Shear
  • Position controlled test at a rate of ≤25mm/min
  • Sampled positioned at either 45° or 27° to the table plane
  • Test until functional or mechanical failure (sample yielding)
  • Test results for 5 samples must be obtained
  • Load controlled test
  • Test run to functional or mechanical failure or 5 million cycles
  • Frequency can be determined by the user but must avoid self-heating of the polyacetal tests blocks and specimen. Typically values range from 5–30 Hz in air and up to 1 Hz for in vivo conditions
  • An R ratio of 10 is used (e.g. between 100 N and 1000 N)
  • The maximum test force should represent either 25%, 50% or 75% of the sample yield strength determined from the static tests. Typical maximum forces can be in excess of 2500N
  • Samples should be examined without removal at regular intervals during the tests to check for mechanical failures
Torsion Testing
  • Position controlled test at a rate up to 60°/min
  • Test until functional or mechanical failure (sample yielding)
  • A compressive pre-load of either 100N, 300N or 500N depending on the implant type*, is required to prevent separation of the assembly

*Cervical (100N), thorasic (300N) and lumber (500N)

  • Torque controlled test
  • Test run to functional or mechanical failure or 5 million cycles
  • Frequency can be determined by the user but must avoid self-heating of the polyacetal tests blocks and specimen. Typically, up to 10 Hz in air and 1 Hz for in vivo conditions
  • An R value of –1 is used for the torsional testing (e.g. between 3Nm and -3Nm)
  • Samples should be examined without removal at regular intervals during the tests to check for mechanical failures

TEST RESULTS

For the Static axial tests, a force vs. displacement curve is produced. Values for mechanical and material properties are then presented in a table showing the mean and standard deviation across a minimum of five samples.

ASTM F2077 Screen Test Results Graph

A simple Load vs. Displacement plot is used to characterise each sample for the Static tests.

Static Test Results Table (ASTM F2077)

Specimen ID Stiffness (N/mm) Yield Displacement (mm) Yield Load (N) Ultimate Displacement (mm) Ultimate Load (N)
Sample 1 10,134 1.32 11,218 1.74 14,238
Sample 2 10,865 1.30 11,435 1.73 15,387
Sample 3 11,012 1.27 11,562 1.69 13,890
Sample 4 10,962 1.29 11,021 1.58 14,327
Sample 5 10,377 1.31 10,934 1.67 15,764
Mean 10,670 1.30 11,234 1.68 14,721
St. Dev 350.26 0.02 238.16 0.06 722.56

The data for a minimum of five samples is shown in a table format with the Mean and Standard Deviation shown for each column.

For the Static torsion tests, a torque vs. angle curve is produced instead with a similar table providing the same mean and standard deviation values.
For the Dynamic tests, an SN curve with a minimum of 6 points is required for each specimen type, the aim being to identify the endurance life stress.

Dynamic Test Results Table (ASTM F2077)

Specimen ID Maximum Load (N) Minimum Load (N) Number of Cycles Achieved Failure Mode
Sample 1 5,000 500 1,004,572 Fracture
Sample 2 4,000 400 4,000,000 Fracture
Sample 3 3,000 300 5,000,000 Pass without Fracture
Sample 4 2,000 200 5,000,000 Pass without Fracture
Sample 5 1,000 100 5,000,000 Pass without Fracture

Dynamic Test data is summarised in a table for each sample.

Test Results Graph

The data point from each sample can be used to produce a plot of Stress vs. No. of cycle to failure.

 